Product
Showroom |
 |
| Characteristic Magnetic Properties
of SmCo Magnets |
| |
| |
| Material |
Grade |
Remanence |
Coercivity |
Intrinsic Coercivity |
Energy Density |
Courier |
Maximum Working Temperature |
| |
|
|
|
|
|
Force |
Product Bhm |
Temperature |
Temperature |
| |
|
Br |
bHc |
iHc |
(BH)max |
TC |
TW |
| |
|
T |
KGs |
KA/m |
KOe |
KA/m |
KOe |
KJ/m3 |
MGOe |
°C |
°C |
| Sintered |
| |
YX-18 |
0.85-0.9 |
8.5-9.0 |
620-648 |
7.8-8.2 |
1194-1513 |
15-19 |
127-143 |
16-18 |
750 |
250 |
| SmCo (1:5) |
YX-20 |
0.92-0.96 |
9.2-9.6 |
653-717 |
8.2-9.0 |
1194-1513 |
15-19 |
150-167 |
19-21 |
750 |
250 |
| |
YX-24 |
0.96-1.0 |
9.6-10.2 |
730-770 |
9.2-9.7 |
1194-1513 |
15-19 |
175-190 |
22-24 |
750 |
250 |
| |
|
|
|
|
|
|
|
|
|
|
|
| |
YXG-24 |
0.95-1.02 |
9.5-10.2 |
637-732 |
8.0-9.2 |
1433-1990 |
18-25 |
175-190 |
22-24 |
800 |
350 |
| SmCo (2:17) |
YXG-26 |
1.02-1.05 |
10.2-10.5 |
748-796 |
9.4-10.0 |
1433-1990 |
18-25 |
195-215 |
24-26 |
800 |
350 |
| |
YXG-28 |
1.05-0.08 |
10.5-10.8 |
756-796 |
9.5-10.0 |
1433-1831 |
18-25 |
205-220 |
26-28 |
800 |
350 |
| |
YXG-28B |
1.02-1.10 |
10.2-11.0 |
420 |
5.2-5.6 |
440-520 |
5.5-6.5 |
205-220 |
26-28 |
800 |
350 |
| |
YXG-30 |
1.08-1.10 |
10.8-11.0 |
780 |
9.8-10.5 |
955-1195 |
18-25 |
220-240 |
28-30 |
800 |
350 |
| |
YXG-30B |
1.08-1.15 |
10.8-11.5 |
420 |
5.2-5.6 |
440-520 |
5.5-6.5 |
220-240 |
28-30 |
800 |
350 |
| Bonded |
| |
Yb-6 |
0.4 |
4.0 |
280 |
3.5 |
800 |
10 |
30-50 |
4-6 |
- |
120 |
| SmCo (1£º5) |
Yb-10 |
0.5 |
5.0 |
320 |
4.0 |
800 |
10 |
50-65 |
6-8 |
- |
120 |
| |
YbG-10 |
0.6 |
6.0 |
360 |
4.5 |
800 |
10 |
65-80 |
8-10 |
- |
120 |
| SmCo (2:17) |
YbG-12 |
0.7 |
7.0 |
400 |
5.0 |
800 |
10 |
85-95 |
10-12 |
- |
120 |
|
| |
| |
| |
| |
| Ningbo
Ketian Magnet Co,.Ltd |
| No.1 ChengXi(west)
Road,
Cicheng Ningbo,
China 315034
|
| Tel:086-0574-
87574058 (International),
87574888,
87574056,
87574145,87574063,87597567 |
| Fax:086-0574-
87597123,
87574285 |
| Web Site:http://www.ktmagnet.com |
| E-mail:sales@ktmagnet.com
|
|